化工进展 ›› 2017, Vol. 36 ›› Issue (09): 3514-3522.DOI: 10.16085/j.issn.1000-6613.2017-0141

• 资源与环境化工 • 上一篇    下一篇

基于硅基的垃圾焚烧飞灰中温热处理重金属稳固化实验

孙立, 吴新, 刘道洁, 李军辉, 李诗, 都艺伟   

  1. 东南大学能源热转换及其过程测控教育部重点实验室, 江苏 南京 210096
  • 收稿日期:2017-01-20 修回日期:2017-04-05 出版日期:2017-09-05 发布日期:2017-09-05
  • 通讯作者: 吴新,副教授,研究方向为高效清洁燃烧与污染物控制排放技术、流化床燃烧与气化、多相流传热流动、测试技术等。
  • 作者简介:孙立(1992-),男,硕士研究生,研究方向为垃圾焚烧飞灰稳固化
  • 基金资助:
    国家重点研发计划项目(2016YFB0600602)。

Stabilization of heavy metals in municipal solid waste incineration fly ash using thermal treatment with silica-based material

SUN Li, WU Xin, LIU Daojie, LI Junhui, LI Shi, DU Yiwei   

  1. Key Laboratory of Energy Thermal Conversion and Process Control of Ministry of Education, Southeast University, Nanjing 210096, Jiangsu, China
  • Received:2017-01-20 Revised:2017-04-05 Online:2017-09-05 Published:2017-09-05

摘要: 向垃圾焚烧飞灰(MSWI FA)中分别添加硅灰、硅溶胶、石英砂与一定比例的水,混合均匀并进行热处理。研究了添加物种类、热处理温度对垃圾焚烧飞灰中重金属浸出特性的影响,分析了飞灰热处理过程中重金属化学形态、晶体结构和微观形貌的变化。结果表明:热处理过程中,硅灰和硅胶与飞灰中的钙基物质反应生成CaSiO3、Ca2SiO4、Ca3SiO4Cl2、Ca3Fe2(SiO43以及氢氧硅磷灰石等硅酸盐相,转变了重金属的化学形态,将重金属稳固在硅酸盐晶格中,降低了飞灰的浸出毒性;在硅灰添加量为10%或JN-40硅胶添加量25%,热处理温度600℃条件下,热处理1h后,飞灰中Pb的浸出浓度由11.91mg/L分别降至0.79mg/L和0.78mg/L,Cd的浸出浓度由3.18mg/L分别降至0.09mg/L和0.10mg/L;热处理过程中Cr的浸出浓度有所上升但未超出生活垃圾填埋场控制标准。

关键词: 垃圾焚烧, 飞灰, 热处理, 重金属, 稳固化

Abstract: Heat treatments were performed with municipal solid waste incineration fly ash(MSWI FA),mixing with silica fume,colloidal silica,quartz sand respectively and a certain proportion of water. The effects of additive species,thermal treatment temperature on the leaching of critical heavy metals(Pb,Cd and Cr) were studied. The changes of chemical speciation of heavy metals,crystal structure and microstructure during heat treatment were also investigated. The results showed that silica fume and colloidal silica react with calcium-based materials in fly ash to form silicate phases such as CaSiO3、Ca2SiO4、Ca3SiO4Cl2、Ca3Fe2(SiO4)3 and hydroxyl-ellestadite during the heat treatment,changing the chemical speciation of heavy metals and stabilizing heavy metals in the silicate lattice,which reduces the leaching toxicity. The leaching concentration of Pb in fly ash decreased from 11.91mg/L to 0.79mg/L and 0.78mg/L,respectively,under the conditions of adding 10% silica fume or 25% JN-40 colloidal silica and heat treatment at 600℃ for one hour,while the leaching concentration of Cd decreased from 3.18mg/L to 0.09mg/L and 0.10mg/L,respectively. During the heat treatment,the leaching concentration of Cr increased but did not exceed the standard for pollution control on the landfill site of municipal solid waste.

Key words: municipal solid waste incineration, fly ash, thermal treatment, heavy metals, stabilization and solidification

中图分类号: 

京ICP备12046843号-2;京公网安备 11010102001994号
版权所有 © 《化工进展》编辑部
地址:北京市东城区青年湖南街13号 邮编:100011
电子信箱:hgjz@cip.com.cn
本系统由北京玛格泰克科技发展有限公司设计开发 技术支持:support@magtech.com.cn